Team:HokkaidoU Japan/Notebook/plastic protocols
From 2012.igem.org
Polymer producing media
polymer producing media (LB:2%Glc+ 10mM pantothenic acid Ca + Amp100mg/l) 20ml
2×LB | 10ml |
●50% Glucose | 800ul |
●1M pantothenic acid Ca | 200ul |
Amp(100mg/ml) | 20ul |
ROwater | 8.98ml |
Put 1.5ml each into the test tube.
●50%gulcose
ROwater | 7ml |
Glucose | 10g Heat until it melts. |
ROwater | up to 20ml |
Filter sterilize.
●1M pantothenic acid Ca
ROwater | 7ml |
pantothenic acid Ca | 4.77g Heat and stir until it melts. |
ROwater | up to 10ml |
Filter sterilize.
Polymer extraction and purification
- Move dried up bacteria into test tube.
- Break up them to separate and add 10ml chloroform.
- Incubate for 48hour at 60C.
- Make it filtered through PTFE and move it into another test tube.
- Volatilize organic solvent by exposing air and separate polymer.
- Add 5ml hexane and voltex for a minute. After centrifuging (1,500rpm, 10min), remove the clear layer.
- Volatilize chloroform by exposing air again.
- Add 5ml MtOH, voltex for a minute, centrifuge (1,500rpm, 10min), and remove the clear layer.